Company Profile What is a Ferrite? Manufacturing Process Products Quality Assurance Capabilities What's New Career Opportunities Tech Alerts Contact Us Home
Manganese-Zinc Ferrites for Industrial
and Professional Applications

    Applications guide   Power/Switching
Transformers, Differential Mode Chokes
Output Chokes
  Wideband Transformers, Pulse Transformers, Common Mode Chokes
Current Sensing Devices,
RFI Suppression
Parameter   Symbol   Standard Conditions
of Test
  Unit   F47   F44   F5   F5A   F6   F9   F9C   F10   F57   F39   F8   P10   P11   P12   F58   FB2   FB3   F9Q   F9N   F65*   F82   FT6   FT7   FTA
Initial Permeability
(nominal)
  µi   B<0.1mT  10kHz
25°C
  -   1800
± 20%
  1900
± 20%
  2000
± 20%
  2500
± 20%
  1800
± 20%
  4400
± 20%
  5000
± 20%
  6000
± 20%
  7500
± 25%
  10000
± 30%
  1200
  min
  2000
± 20%
  2250
± 20%
  2000
± 20%
  750
± 20%
  2000
± 20%
  2700
± 20%
  2300
± 20%
  4000
± 20%
  4400
± 40%
  5000
± 20%
  6000
± 20%
  7500
± 25%
  10000
± 30%
Saturation Flux
Density (typical)
  Bsat   H=796 A/m  10 Oe
25°C  Static  100°C
  mT   470
350
  500
400
  470
350
  470
350
  350
-
  380
-
  460
-
  380
-
  380
-
  380
-
  380
-
  -
-
  -
-
  -
-
  >420   480   480   350*
-
  410
-
  350   460   430   420   420
Remanent Flux
Density (typical)
  Br   H–›0 (from near saturation)
10 kHz 25°C
  mT   130   270   200   150   -   180   170   100   250   200   -   120   70   35   -   140   140   190   270   100   170   150   130   180
Coercivity (typical)   Hc   B–›0 (from near saturation)
10 kHz 25°C
  A/m   24   27   21   15   -   13   13   14   17   16   -   22   18   7   -   10   10   24   15   14   13   15   10   8
Loss
Factor
(maximum)
  Loss Factor Equation     B<0.1mT  25°C
10 kHz
100 kHz
200 kHz
1 MHz
  10-6   -
-
-
-
  -
-
-
-
  -
-
-
-
  -
-
-
-
  -
-
-
-
  -
20
-
-
  -
20
-
-
  -
20
-
-
  -
-
-
-
  -
-
-
-
  -
-
-
-
  6
15
-
-
  1.5
5
-
-
  0.8
2.5
-
-
  -
-
-
-
  30
-
-
-
  15
-
-
-
  -
20
-
-
  -
30
-
-
  -
20
-
-
  -
20
-
-
  -
25
  6
50
-
-
  6
50
-
-
Temperature Factor   Temperature Factor Equation   B<0.1mT  10kHz
+25°C to +55°C
B<0.1mT 10kHz
0°C to +25°C
  10-6/°C   -
 
-
  -
 
-
  -
 
-
  -
 
-
  -
 
-
  0 to 2
 
-
  -1 to +2
 
-
  -1 to +2
 
-
  -
 
-
  -
 
-
  -
 
-
  0 to 2
 
-
  .5 to 1.5
 
-
  .4 to 1.0
 
-
  -
 
-
  -
 
-
  -
 
-
  -
 
-
  -
 
-
  -
 
-
  -1 to +2
 
-
  -
 
-
  -
 
-
  -1 to 0
 
-0.5 to +0.5
Curie Temperature (minimum)   TC   B<0.1mT  10kHz   °C   200   230   200   200   180   130   160   130   125   125   130   150   150   150   310   230   230   140   150   >150   160   140   150   150
Disaccomodation
Factor (max)
  equation   B<0.25mT   10kHz
50°C   10 to 100 mins
  10-6   -   -   -   -   -   -   -   -   -   -   -   8   4   3   -   -   -   -   -   -   -   -   -   -
Hysteresis Material
Constant (max)
  equation   B from 1.5 to 3mT  10kHz
25°C
  10-6/mT   -   -   -   -   -   -   -   -   -   -   -   2.4   0.8   0.45   -   -   -   -   -   -   -   -   -   -
Resistivity (typical)     1V/cm   25°C   omega-cm   100   100   100   100   100   50   50   50   100   100   100   100   100   100   100   100   100   20   20   20   50   20   10   10
Amplitude
Permeability
(minimum)
  µa   400mT   25°C
 320mT   100°C
 340mT   100°C
  µa   -
-
-
  2500
-
1900
  2500
-
1900
Total Power
Loss Density
(maximum)
  Pv   200mT;   16kHz :  25°C
200mT;   16kHz :  60°C
200mT;   16kHz :  100°C
200mT;   25kHz :  25°C
200mT;   25kHz :  60°C
200mT;   25kHz :  100°C
100mT;   100kHz :  25°C 100mT;   100kHz :  100°C 200mT;   100kHz :  100°C 50mT;   400kHz :  25°C 50mT;   400kHz :  100°C
  mW/cc   -
-
-
-
-
-
-
-
-
-
-
  -
-
-
200
-
130
250
160
750
-
-
  -
-
-
200
-
130
250
160
750
-
-
  * Bsat measured at H=1200 A/m
Bsat measured at H=4000 A/m